1. 30CrMnSiA steel plate has excellent workability, small deformation and good fatigue resistance.
2. Chemical composition of 30CrMnSiA steel plate:
Carbon C: 0.28-0.34 
Silicon Si: 0.90-1.20 
Manganese Mn: 0.80-1.10 
Sulfur S: Allow remaining content ≤0.025 
Phosphorus P: Allow remaining content ≤0.025 
Chromium Cr: 0.80-1.10 
Nickel Ni: Allow remaining content ≤0.030 
Copper Cu: Allow remaining content ≤0.025
3. Mechanical properties of 30CrMnSiA steel plate: 
Tensile strength σb (MPa): ≥1080(110) 
Yield strength σs (MPa): ≥835(85) 
Elongation δ5 (%): ≥10 
Section shortening rate ψ (%): ≥45 
Impact energy Akv (J): ≥39 
Impact toughness value αkv (J/cm²): ≥49(5) 
Hardness: ≤229HB 
Sample size: sample blank size is 25mm
4. Heat treatment standard and metallographic arrangement: 
Heat treatment standard: quenching 880℃, oil cooling; tempering 540℃, water cooling, oil cooling.